  • asciidoc
  • rtf
Laser Powder Bed Fusion of Ti-6Al-4V for Industrial Applications: Balancing Productivity and Mechanical Properties
University West, Department of Engineering Science, Division of mechanical engineering. (KAMPT)ORCID iD: 0000-0003-2857-7154
2026 (English)Doctoral thesis, comprehensive summary (Other academic)Alternative title
Laserbaserad Pulverbäddsfusion av Ti-6Al-4V för industriella tillämpningar : avvägning mellan produktivitet och mekaniska egenskaper (Swedish)
Abstract [sv]

Additiv tillverkning (AM) möjliggör tillverkning av komplexa metalliskakomponenter direkt från digitala modeller, med minskat materialspilloch kortare väg från konstruktion till färdig komponent. Bland metallbaseradeAM tekniker har laserbaserad pulverbäddsfusion (PBF-LB) fåttett betydande industriellt genomslag. Samtidigt begränsas en bredareimplementering fortfarande av relativt låg produktivitet, kostnader koppladetill pulverråvaran och behovet av efterbearbetning för att uppnåerforderlig materialkvalitet.

Denna avhandling undersöker strategier för att öka produktiviteten vid PBF-LB-bearbetning av Ti-6Al-4V utan att försämra de mekaniska egenskaperna. En bred partikelstorleksfördelning på 15–90 μm kombinerades med en lagertjocklek på 70μm, och ett processfönster fastställdes genom att studera effekten av lasereffekt, skanningshastighet och spåravstånd på smältbad, konsolidering och defektbildning.

Resultaten visar att den bredare partikelstorleksfördelningen kan bearbetas framgångsrikt vid ökad lagertjocklek när processparametrarna anpassas på lämpligt sätt.

  Två processstrategier studerades vidare: en med minimal porositet och en med hög produktivitet. Den högproduktiva strategin uppvisade lägre duktilitet och slagseghet i byggtillståndet till följd av bristande sammansmältning. Varmisostatisk pressning (HIP) användes därför både för konsolidering och mikrostrukturstyrning. HIP under β-transustemperaturen reducerade interna defekter och bibehöll en relativt fin mikrostruktur med hög duktilitet. HIP över β-transustemperaturen gav grövre tidigare β-korn och större α-kolonier, vilket förbättrade slagseghet och motstånd mot utmattningsspricktillväxt men minskade draghållfasthet och motstånd mot utmattningssprickinitiering.

Programmerbar laserstråleformning undersöktes även som ett verktyg för att påverka de termiska förhållandena under bearbetningen. Sammantaget visar avhandlingen att ökad PBF-LB-produktivitet kan uppnås genom en kombination av bredare partikelstorleksfördelning, ökad lagertjocklek, anpassade processparametrar och riktad efterbearbetning. Resultaten visar att produktivitet, defektpopulation, mikrostruktur och mekaniska egenskaper behöver betraktas som integrerade delar av samma tillverkningskedja.

Abstract [en]

Additive Manufacturing has transformed the production of metallic components by enabling complex geometries to be manufactured directly from digital models while reducing material waste and shortening the design-to-manufacture route. Among metal AM technologies, laser powder bed fusion (PBF-LB) has gained considerable industrial interest, particularly in the biomedical, automotive and aerospace sectors. Despite these advantages, wider industrial adoption remains constrained by relatively low build rates, feedstock optimisation costs and the need to consistently achieve the material quality required for structural applications by adding post processing.

This thesis investigates strategies for increasing the productivity of PBF-LB processing of Ti-6Al-4V while maintaining suitable mechanical properties. A wide powder particle size distribution of 15-90 μm was combined with an increased layer thickness of 70 μm, and a specific processing window was established by evaluating the effects of laser power, scanning speed and hatch distance on melt pool behaviour, consolidation and defect formation. The results show that the wider powder distribution can be successfully processed at increased layer thickness, provided that the process parameters are appropriately adapted.

Two representative processing strategies were subsequently investigated: a minimal porosity and a high productivity condition. The latter showed reduced ductility and impact toughness in the as-built condition due to lack-of-fusion defects. Hot Isostatic Pressing (HIP) was therefore investigated both as a consolidation method and as a means of tailoring the microstructure. Sub-β transus HIP effectively consolidated internal defects while retaining a comparatively refined microstructure and promoting high ductility. HIP above the β transus produced coarser prior-β grains and larger α colonies, improving impact toughness and fatigue crack growth resistance but reducing tensile strength and resistance to fatigue crack initiation. These findings show that the as-built condition affects not only defect formation but also the microstructure developed during subsequent HIP treatment.

Finally, programmable laser beam shaping was investigated as an additional tool to vary the thermal behaviour during processing.

Overall, the thesis demonstrates that increased PBF-LB productivity can be achieved through the combined use of wider powder particle size distributions, increased layer thickness, adapted process parameters and targeted post processing. The results highlight the need to consider productivity, defect content, microstructure and mechanical performance as an integrated manufacturing chain tailored to the requirements of the intended application.

Place, publisher, year, edition, pages
Trollhättan: University West , 2026. , p. 25
Series
PhD Thesis: University West ; 89
Keywords [en]
Powder Bed Fusion Laser Beam (PBF-LB), Ti-6Al-4V, Microstructure, Particle Size Distribution (PSD), Productivity Enhancement
Keywords [sv]
Pulverbädd additiv tillverkning (PBF-LB/M), Ti-6Al-4V, Mikrostruktur, Pulverpartikelstorleksfördelning, Produktivitetsförbättring
National Category
Manufacturing, Surface and Joining Technology
Identifiers
URN: urn:nbn:se:hv:diva-26329ISBN: 9789189969865 (print)ISBN: 9789189969858 (print)OAI: oai:DiVA.org:hv-26329DiVA, id: diva2:2109021
Public defence
2026-11-12, F210, Gustava Melins gata, Trollhättan, 09:00 (English)
Opponent
Supervisors
Note

Paper B and E are to be submitted and not included in the electronic thesis.

Available from: 2026-10-20 Created: 2026-10-08
List of papers
1. Extending powder particle size distribution of laser powder bed fusion Ti-6Al-4V: investigation of single tracks and multilayer experiments
Open this publication in new window or tab >>Extending powder particle size distribution of laser powder bed fusion Ti-6Al-4V: investigation of single tracks and multilayer experiments
Show others...
2023 (English)Conference paper, Oral presentation with published abstract (Other academic)
Abstract [en]

This paper explores the effects of varying process parameters (i.e., laser power, laser scanning speed, hatch distance) on the characteristics of single tracks, triple tracks and cubes, in order to provide answers to Research Question 1. A full factorial DoE approach was adopted to produce the experiments. Data was extracted from different sources to find correlations between tracks and multilayer geometries. A digital microscope was used to obtain height profiles, whilst polished/etched cross sections cut parallel to the build direction were imaged using a LOM to obtain measurements of track height, width, melt pool depth, subsurface porosity and residual defect content in cubes. Track height was found to exceed the recoated value of 70μm for both single and triple tracks. The width of single tracks showed a clear upward trend when displayed against VED, showing a lateral expansion as energy input increased. It was also revealed that single tracks expand laterally as they grow above the substrate, indicating swelling. The melt pool depth showed a steady upward trend when plotted against LED, though less systematic than track width. A martensitic microstructure was detected, with hierarchical α’ needles growing at prescribed crystallographic directions within vertical prior-β grains. A large portion of spatter particles and unmelted powder granules were detected on the substrate and tracks, with many accumulating on the side of the tracks forming a denudation zone.

Keywords
extendign powder, laser powder
National Category
Manufacturing, Surface and Joining Technology
Research subject
Production Technology
Identifiers
urn:nbn:se:hv:diva-20988 (URN)
Conference
15th World Titanium Conference, June 2023, Edinburgh, United Kingdom
Note

This paper is under review och will be published in Proceedings.

Available from: 2023-11-24 Created: 2023-11-24 Last updated: 2026-10-08Bibliographically approved
2. Microstructure and mechanical properties of Ti-6Al-4V alloy fabricated using powder bed fusion: laser beam additive manufacturing process: Effect of hot isostatic pressing
Open this publication in new window or tab >>Microstructure and mechanical properties of Ti-6Al-4V alloy fabricated using powder bed fusion: laser beam additive manufacturing process: Effect of hot isostatic pressing
Show others...
2025 (English)In: Materials Science & Engineering: A, ISSN 0921-5093, E-ISSN 1873-4936, Vol. 931, p. 1-19, article id 148226Article in journal (Refereed) Published
Abstract [en]

Powder bed fusion laser beam (PBF-LB) is one of the most widespread and highly researched additive manufacturing (AM) methods, spanning multiple industries. Its feedstock material is metallic powder, where a conventional particle size range is 15–50 μm. The present study focuses on Ti-6Al-4V powder with a wider particle size distribution (15–90 μm). Two process themes are evaluated: one minimising porosity and one maximising build rate through a fast laser scanning speed. The effect of two hot isostatic pressing (HIP) heat treatments on mechanical properties, one below and one above the β-transus, are compared to those of as-built and stress relieved material. Room temperature impact toughness and tensile testing are used to compare the materials by determining UTS and Yield strength, elongation and reduction of area for the different process conditions and post build heat treatments. The minimal porosity theme reaches properties comparable to conventional manufacturing processes at all heat treatment temperatures (i.e., UTS >860 MPa, 0.2 % Yield >795 MPa). The high productivity theme treated below β-transus provides further improvement in overall reduction of area (>45 %) and elongation (>20 %) with respect to the minimal porosity theme, by showing a bi-modal microstructure that is the result of a recrystallisation process. This phenomenon is triggered by the closure of lack of fusion (LoF) defects via hot isostatic pressing, due to a higher dislocation density at the tip of these particular defects. Impact energy for this condition increases whilst hardness and texture become less pronounced. It is demonstrated that in those cases where a fast scanning speed creates LoF defects, those can assist in modifying microstructure during the consolidation process which has a positive effect on ductility.

Keywords
Ti-6Al-4V Powder size distribution Productiv, ity enhancement, Hot isostatic pressing heat treatment (HIP), Microstructure
National Category
Manufacturing, Surface and Joining Technology
Research subject
Production Technology
Identifiers
urn:nbn:se:hv:diva-23329 (URN)10.1016/j.msea.2025.148226 (DOI)001468465500001 ()2-s2.0-105000391412 (Scopus ID)
Note

CC BY 4.0

Available from: 2025-05-07 Created: 2025-05-07 Last updated: 2026-10-08
3. Influence of sub/super- β transus HIP treatments on the fatigue crack initiation of PBF-LB Ti-6Al-4V produced with varying defect content
Open this publication in new window or tab >>Influence of sub/super- β transus HIP treatments on the fatigue crack initiation of PBF-LB Ti-6Al-4V produced with varying defect content
2026 (English)In: International Journal of Fatigue, ISSN 0142-1123, E-ISSN 1879-3452, Vol. 209, p. [1-19], article id 109654Article in journal (Refereed) Published
Abstract [en]

Hot isostatic pressing (HIP) is commonly applied to additively manufactured Ti-6Al-4V to eliminate lack-of-fusion (LoF) defects; however, significant differences in fatigue performance are often observed even when residual porosity is comparable. This study investigates whether fatigue behaviour in PBF-LB Ti-6Al-4V material with varying defect content is controlled by process defects or by microstructure-dependent crack initiation mechanisms. Specimens were produced using two process themes, a minimal porosity (MP) and a high productivity (HP) condition with reduced volumetric energy input, and subsequently HIP treated below or above the -transus temperature. X-ray computed tomography confirmed that HIP effectively healed LoF defects in the HP material, reducing residual porosity to levels comparable to MP builds. Fatigue testing revealed that, once defects were eliminated, fatigue life depended strongly on the HIP microstructure: sub- HIP consistently produced longer lives than super- HIP across all stress levels. EBSD analysis showed that sub- HIP generated a fine  structure that distributed cyclic plasticity across many grains, whereas super- HIP formed large prior- grains containing coarse  colonies with very fine lamellar structure within each colony. These colonies acted as microstructural units, concentrating cyclic slip into long bands and promoting early crack initiation. The results show that HIP reduces defect density and the remaining fatigue failures are predominantly governed by microstructural mechanisms. After excluding a few samples with defect initiated failures, fatigue life was controlled by colony slip localisation, identifying the  colony size as the dominant microstructural fatigue length scale. Tailoring HIP temperature provides a route to achieving wrought-comparable fatigue performance in high-productivity PBF-LB Ti-6Al-4V.

Keywords
Powder bed fusion laser beam, Hot isostatic pressing, Uniaxial fatigue, Productivity enhancemen, tPowder particle size distribution
National Category
Manufacturing, Surface and Joining Technology
Research subject
Production Technology
Identifiers
urn:nbn:se:hv:diva-25066 (URN)10.1016/j.ijfatigue.2026.109654 (DOI)001733945500001 ()2-s2.0-105034123251 (Scopus ID)
Note

CC BY 4.0

Available from: 2026-05-28 Created: 2026-05-28 Last updated: 2026-10-08
4. A comprehensive framework to study the influence of beam shaping in laser metal fusion processes
Open this publication in new window or tab >>A comprehensive framework to study the influence of beam shaping in laser metal fusion processes
Show others...
2025 (English)In: Materials & design, ISSN 0264-1275, E-ISSN 1873-4197, Vol. 259, article id 114805Article in journal (Refereed) Published
Abstract [en]

Beam shaping is considered a technology capable of dramatically improving quality and robustness of Laser Metal Fusion (LMF) processes. However, systematic investigations of its effects on melt-pool dynamics, temperature field and microstructure are still required. In this work, we propose an integrated approach combining a Computational Fluid Dynamics (CFD) model, in-situ temperature measurements and metallographic analysis to explore programmable ring beam profiles, ranging from Gaussian-dominant to ring-dominant configurations. This method, initially proposed on Ti-6Al-4V bead-on-plate tracks, validates melt-pool temperatures measured in-process by a dual-wavelength pyrometer against CFD predictions, which are in turn validated with metallographic cross-sections. Ring modes lowered peak temperature by up to 35 %, transforming deep-narrow pools (aspect ratio approximate to 0.9) into shallow-wide ones (approximate to 0.4). This suppressed humping at line energies >= 0.28 J mm-1, whereas lower energies produced only superficial melting. Simulations matched pyrometer data within 5 % whenever pool width equalled the pyrometers’ sensing spot; all tracks solidified into ultrafine alpha with retained beta, independent of beam mode. Therefore, the combination of in-situ, ex-situ and CFD tools offers a practical workflow for assisting data-driven process optimization and can be easily extended to other LMF processes, with its potential implementation in industrial Laser Powder Bed Fusion.

Place, publisher, year, edition, pages
Elsevier, 2025
Keywords
Dual-wavelength pyrometry; CFD simulations; Ti-6Al-4V; Laser Metal Fusion (LMF); Beam shaping; Electron Backscatter Diffraction (EBSD)
National Category
Manufacturing, Surface and Joining Technology
Research subject
Production Technology
Identifiers
urn:nbn:se:hv:diva-24456 (URN)10.1016/j.matdes.2025.114805 (DOI)001582316500003 ()2-s2.0-105020860737 (Scopus ID)
Funder
Swedish Research Council, 2022-06725
Note

CC-BY 4.0 

The computations and related data handling were enabled by resources provided by the National Academic Infrastructure for Supercomputing in Sweden (NAISS), partially funded by the Swedish Research Council through grant agreement no. 2022-06725.

Available from: 2026-01-09 Created: 2026-01-09 Last updated: 2026-10-08

Open Access in DiVA

Avhandlingen(19436 kB)86 downloads
File information
File name FULLTEXT01.pdfFile size 19436 kBChecksum SHA-512
3e2951c33b40d3f83f8efeb7a005f468f31b3b9aabf75036cb7214f7011e17273ea1634bce07a22fd0ca27f4dee8fa42dabdc529ce03708e00821ad230920ef6
Type fulltextMimetype application/pdf
Spikbladet(36 kB)20 downloads
File information
File name FULLTEXT02.pdfFile size 36 kBChecksum SHA-512
12e4c9a60da7eea390168fef128b7337c55b0b36f47a984eef0f143352e647e79c329bda0fc2445ecc90098274243a0729fadb992daa3687ed37b4958fbe1dfa
Type spikbladMimetype application/pdf

Authority records

Squillaci, Linda

Search in DiVA

By author/editor
Squillaci, Linda
By organisation
Division of mechanical engineering
Manufacturing, Surface and Joining Technology

Search outside of DiVA

GoogleGoogle Scholar
Total: 106 downloads
The number of downloads is the sum of all downloads of full texts. It may include eg previous versions that are now no longer available

isbn
urn-nbn

Altmetric score

isbn
urn-nbn
Total: 29715 hits
CiteExportLink to record
Permanent link

Direct link
Cite
Citation style
  • apa
  • ieee
  • modern-language-association-8th-edition
  • vancouver
  • Other style
More styles
Language
  • de-DE
  • en-GB
  • en-US
  • fi-FI
  • nn-NO
  • nn-NB
  • sv-SE
  • Other locale
More languages
Output format
  • html
  • text
  • asciidoc
  • rtf